1.0119 (S235J2G4C)

Classification

Country Section Category
Germany Non-alloy Steels Quality Steel (General Structural Steels with Rm < 500 MPa)

Chemical composition

Standard Fe, % Mn, % P, % C, % S, % N, %
EN 10025 > 98.351 < 1.4 < 0.035 < 0.17 < 0.035 < 0.009

Information on suppliers

Properties

Property
According to EN 10025-2 Thickness: < 16 mm ; yield strength: > 235 MPa
According to EN 10025-2 Thickness: < 16 mm ; yield strength: 350 - 510 MPa
According to EN 10025-2 Thickness: 16 - 40 mm ; yield strength: > 225 MPa
According to EN 10025-2 Thickness: 16 - 40 mm ; tensile strength: 350 - 510 MPa
According to EN 10025-2 Thickness: 40 - 100 mm ; yield strength: > 215 MPa
According to EN 10025-2 Thickness: 40 - 100 mm ; tensile strength: 350 - 510 MPa
According to EN 10025-2 Thickness: 100 - 150 mm ; yield strength: > 195 MPa
According to EN 10025-2 Thickness: 100 - 150 mm ; tensile strength: 350 - 500 MPa
According to EN 10025-2 Thickness: 150 - 200 mm ; yield strength: > 185 MPa
According to EN 10025-2 Thickness: 150 - 200 mm ; yield strength: 240 - 490 MPa
According to EN 10025-2 Thickness: 200 - 250 mm ; yield strength: > 175 MPa
According to EN 10025-2 Thickness: 200 - 250 mm ; tensile strength: 340 - 490 MPa
According to EN 10025-2 Thickness: > 250 mm ; yield strength: > 165 MPa
According to EN 10025-2 Thickness: > 250 mm ; tensile strength: 330 - 480 MPa
According to EN 10025-2 Longitudinal samples Thickness: < 1 mm ; elongation: > 17 %
According to EN 10025-2 Longitudinal samples Thickness: 1.0 - 1.5 mm ; elongation: > 18 %
According to EN 10025-2 Longitudinal samples Thickness: 1.5 - 2.0 mm ; elongation: > 19 %
According to EN 10025-2 Longitudinal samples Thickness: 2.0 - 2.5 mm ; elongation: > 20 %
According to EN 10025-2 Longitudinal samples Thickness: 2.5 - 3.0 mm ; elongation: > 21 %
According to EN 10025-2 Longitudinal samples Thickness: 3 - 40 mm ; elongation: > 26 %
According to EN 10025-2 Longitudinal samples Thickness: 40 - 63 mm ; elongation: > 25 %
According to EN 10025-2 Longitudinal samples Thickness: 63 - 100 mm ; elongation: > 24 %
According to EN 10025-2 Longitudinal samples Thickness: 100 - 150 mm ; elongation: > 22 %
According to EN 10025-2 Longitudinal samples Thickness: 150 - 250 mm ; elongation: > 21 %
According to EN 10025-2 Longitudinal sample Thickness: 250 - 400 mm ; elongation: > 21 %
According to EN 10025-2 Transverse specimens Thickness: < 1 mm ; elongation: > 15 %
According to EN 10025-2 Transverse specimens Thickness: 1.0 - 1.5 mm ; elongation: > 16 %
According to EN 10025-2 Transverse specimens Thickness: 1.5 - 2.0 mm ; elongation: > 17 %
According to EN 10025-2 Transverse specimens Thickness: 2.0 - 2.5 mm ; elongation: > 18 %
According to EN 10025-2 Transverse specimens Thickness: 2.5 - 3.0 mm ; elongation: > 19 %
According to EN 10025-2 Transverse specimens Thickness: 3 - 40 mm ; elongation: > 24 %
According to EN 10025-2 Transverse specimens Thickness: 40 - 63 mm ; elongation: > 23 %
According to EN 10025-2 Transverse specimens Thickness: 63 - 150 mm ; elongation: > 22 %
According to EN 10025-2 Transverse specimens Thickness: 150 - 250 mm ; elongation: > 21 %
According to EN 10025-2 Transverse specimens Thickness: 250 - 400 mm ; elongation: > 21 %
According to EN 10025-2 Test for impact strength Thickness: < 150 mm ; Work strike KV at -20°C [-4°F]: > 27 j
According to EN 10025-2 Test for impact strength Thickness: 150 - 250 mm ; Work strike KV at -20°C [-4°F]: > 27 j
According to EN 10025-2 Test for impact strength Thickness: > 250 mm ; Work strike KV at -20°C [-4°F]: > 27 j
According to EN 10025-2 bend Test of the note is Used for bending angle < 90°
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 1.0 - 1.5 mm ; bending Radius: > 1.6 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 1.5 - 2.5 mm ; bending Radius: > 2.5 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 2.5 - 3.0 mm ; bending Radius: > 3 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 3 - 4 mm ; bending Radius: > 6 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 4 - 5 mm ; bending Radius: > 8 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 5 - 6mm ; bending Radius: > 10 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 6 - 7 mm ; bending Radius: > 12 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 7 - 8 mm ; bending Radius: > 16 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 8 - 10mm ; bending Radius: > 20 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal sample Thickness: 10 - 12mm ; bending Radius: > 25 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 12 - 14 mm ; bending Radius: > 28 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 14 - 16 mm ; bending Radius: > 32 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 16 - 18 mm ; bending Radius: > 40 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal samples Thickness: 18 - 20mm ; bending Radius: > 45 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal sample Thickness: 20 - 25mm ; bending Radius: > 55 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging the Longitudinal sample Thickness: 25 - 30 mm ; bending Radius: > 70 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 1.0 - 1.5 mm ; bending Radius: > 1.6 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 1.5 - 2.5 mm ; bending Radius: > 2.5 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 2.5 - 3.0 mm ; bending Radius: > 3 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 3 - 4 mm ; bending Radius: > 5 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 4 - 5 mm ; bending Radius: > 6 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 5 - 6mm ; bending Radius: > 8 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 6 - 7 mm ; bending Radius: > 10 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 7 - 8 mm ; bending Radius: > 12 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 8 - 10mm ; bending Radius: > 16 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 10 - 12mm ; bending Radius: > 20 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 12 - 14 mm ; bending Radius: > 25 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 14 - 16 mm ; bending Radius: > 28 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 16 - 18 mm ; bending Radius: > 36mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 18 - 20mm ; bending Radius: > 40 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 20 - 25mm ; bending Radius: > 50 mm
According to EN 10025-2 bend Test of hot rolled plates, cold flanging Transverse specimens Thickness: 25 - 30 mm ; bending Radius: > 60 mm
According to EN 10025-2 bend Test of hot rolled plates, cold rolled Sheet strip, cold profiling Thickness: < 6 mm ; the bend Test in cold state: r > t
According to EN 10025-2 bend Test of hot rolled plates, cold rolled Sheet strip, cold profiling Thickness: 6 - 8mm ; Test cold bending: r > 1.5 t
Density: 7.85 g / cm3

Analogues

Germany CIS, Russia, Ukraine USA
S235J2C Ст3Гсп-а S235J2C

Standards

Standard Description
EN 10025
DIN EN 10025-2:2004
DIN EN 10025-2:2019

Description of chemical elements

Element Units of measurement Description
Fe % Iron
Mn % Manganese
P % Phosphorus
C % Carbon
S % Sulfur
N % Nitrogen