1211
Hot-rolled sheet steel, designed for magnetic circuits of electrical machines
Hot-rolled sheet steel, designed for magnetic circuits of electrical machines
Standard | Fe, % | Si, % |
---|---|---|
Standard | Fe, % | Si, % |
GOST 21427.3-75 | 98.2–99.2 | 0.8–1.8 |
Rolling | Dimensions, mm | P_{1.0/50}, W/kg | P_{1.5/50}, W/kg | B_{2500}, T | B_{5000}, T | B_{10000}, T | B_{30000}, T |
---|---|---|---|---|---|---|---|
Rolling | Dimensions, mm | P_{1.0/50}, W/kg | P_{1.5/50}, W/kg | B_{2500}, T | B_{5000}, T | B_{10000}, T | B_{30000}, T |
Sheet hot rolled. | 1 | 5.8 | 13.4 | 1.53 | 1.63 | 1.76 | 2 |
Sheet hot rolled. | 0.5 | 3.3 | 7.7 | 1.53 | 1.64 | 1.76 | 2 |
Standard | Description |
---|---|
Standard | Description |
GOST 21427.3-75 |
Parameter | Units of measurement | Description |
---|---|---|
Parameter | Units of measurement | Description |
Dimensions | mm | |
P_{1.0/50} | W/kg | Specific magnetic losses (no more) while the magnetic induction is 1.0 T and frequency is 50 Hz |
P_{1.5/50} | W/kg | Specific magnetic losses (no more) while the magnetic induction is 1.5 T and frequency is 50 Hz |
B_{2500} | T | Magnetic induction (not less) in a magnetic field while magnetic field strength is 2500 A/m |
B_{5000} | T | Magnetic induction (not less) in a magnetic field while magnetic field strength is 5000 A/m |
B_{10000} | T | Magnetic induction (not less) in a magnetic field while magnetic field strength is 10000 A/m |
B_{30000} | T | Magnetic induction (not less) in a magnetic field while magnetic field strength is 30000 A/m |