Alloy aluminum AL28 (AMg5Mts)

Chemical composition

  • Al Aluminum Rest
    Fe Iron <0.25
    Si Silicon <0.3
    Mg Magnesium 4.8 — 6.3
    Mn Manganese 0.4 — 1.0
    Cu Copper <0.3
    Ni Nickel <0.02
    Sn Tin <0.02
    Ti Titanium 0.05 — 0.15
    Zn Zinc <0.02
    Zr Zirconium <0.1
    Ot Total impurities <0.4

Casting methods:
Z — sand casting
B — Lost wax casting
K — chill casting
D — injection molding

Analogs in Germany

EN AW-5456 DIN EN 12392: 2016

EN AW-AlMg5Mn1 DIN EN 12392: 2016

EN AW-5456 DIN EN 12392: 2016 / A1: 2019

EN AW-AlMg5Mn1 DIN EN 12392: 2016 / A1: 2019

5456 DIN EN 4632−002: 2008

EN AW-5456 DIN EN 573−3: 2013

EN AW-AlMg5Mn1 DIN EN 573−3: 2013

EN AW-5456A DIN EN 573−3: 2013

EN AW-AlMg5Mn1 (A) DIN EN 573−3: 2013

EN AW-5456B DIN EN 573−3: 2013

EN AW-AlMg5Mn1 (B) DIN EN 573−3: 2013

EN AW-5556A DIN EN 573−3: 2013

EN AW-AlMg5Mn DIN EN 573−3: 2013

Analogs in Russia

AMg5Mts GOST 1583−93

AL28 GOST 1583−93

AL28Z GOST 1583−93

AL28V GOST 1583−93

AL28 GOST 2685−75

AMg5Mts GOST R 55375−12

AL28 GOST R 55375−12

Analogs in the USA

5456A AA

5456B AA

4177 AMS

4182 AMS

4349 AMS

AMS-A-81596 AMS

AMS-QQ-A-200/7 AMS

AMS-QQ-A-250/20 AMS

AMS-QQ-A-250/9 AMS

QQ-A-250/9 AMS

AA5456 ANSI

SB 209 (5456) ASME SB209

SB 221 (5456) ASME SB221

SB 241 (5456) ASME SB241

B 209 (5456) ASTM B209

B 210 (5456) ASTM B210

B 211 (5056) ASTM B211

B 221 (5456) ASTM B221

B 241 (5456) ASTM B241

B 275 (A 95056) ASTM B275

B 275 (A 95456) ASTM B275

B 316 (5056) ASTM B316

B 548 (5456) ASTM B548

B 744 (5456) ASTM B744

B 745 (5456) ASTM B745

F 1667 (5056) ASTM F1667

A95056 UNS

A95456 UNS

C92610 UNS

5056 Included in 7 standards

5456 Included in 8 standards

For the manufacture of shaped castings. Technical requirements GOST 1583−93 Cast aluminum alloys. Technical conditions GOST 2171−90 Parts, products, semi-finished products and billets of non-ferrous metals and alloys. Designation of the brand GOST 2685−75 Cast aluminum alloys. GOST R 55375−12 grades Primary aluminum and alloys based on it. Stamps

Classification

Country Section Category
CIS, Russia, Ukraine Aluminum, aluminum alloys Foundry aluminum alloys

Chemical composition

Standard Fe, % Si, % Mg, % Mn, % Ti, % Cu, % Zr, % Al, %
GOST 1583-93 < 0.5 < 0.3 4.8–6.3 0.4–1 0.05–0.15 < 0.3 < 0.1 91.85–94.75

Information on suppliers

Mechanical properties at 20 °C

Rolling Standard Size, mm Tension Classifiers $$\sigma _{U}$$, $$MPa$$ $$\epsilon_L$$, % Treatment
Alloy 200–210 3.5–5

Brinell hardness number

Rolling Standard Classifiers Value, HBW
Alloy 55

Analogues

Germany USA
AlMg5 5056A

Standards

Standard Description
GOST 1583-93

Description of chemical elements

Element Units of measurement Description
Fe % Iron
Si % Silicon
Mg % Magnesium
Mn % Manganese
Ti % Titan
Cu % Copper
Zr % Zirconium
Al % Aluminium

Description of mechanical properties

Parameter Units of measurement Description
$$\sigma _{U}$$ $$MPa$$ Ultimate tensile strength
$$\epsilon_L$$ % Elongation at break (longitudinal)