15H2M2FBS
forgings diaphragms, pipes and other parts operating at a steam temperature of 565−580 degrees in front of the turbine.
Classification
| Country |
Section |
Category |
| CIS, Russia, Ukraine |
Heat resistant steels and alloys |
Heat resistant low alloy steel |
Chemical composition
| Standard |
Fe, % |
Si, % |
Mn, % |
Cr, % |
Cu, % |
Ni, % |
V, % |
P, % |
C, % |
S, % |
Nb, % |
Mo, % |
|
93.01–95.34 |
0.7–1 |
0.5–0.8 |
1.8–2.3 |
< 0.3 |
< 0.3 |
0.25–0.4 |
< 0.03 |
0.13–0.18 |
< 0.03 |
0.08–0.15 |
1.2–1.5 |
Information on suppliers
Physical characteristics
| Temperature, °C |
$$E\cdot 10^{9}$$, $$MPa$$ |
$$\alpha\cdot 10^{6}$$, $$K^{-1}$$ |
$$\varkappa$$, $$\frac{W}{m\cdot K}$$ |
$$\rho$$, $$\frac{kg}{m^3}$$ |
$$R\cdot 10^{-6}$$, $$\Omega\cdot m$$ |
| 20 |
224 |
|
|
7850 |
0.45 |
| 100 |
219 |
12 |
34.8 |
|
0.46 |
| 200 |
|
|
34.3 |
|
0.52 |
| 300 |
205 |
|
34.1 |
|
0.6 |
| 400 |
|
14.5 |
33.9 |
|
0.67 |
| 500 |
187 |
|
33.7 |
|
0.77 |
| 600 |
176 |
|
33.5 |
|
0.95 |
| 700 |
164 |
|
|
|
|
Mechanical properties at 20 °C
| Rolling |
Standard |
Size, mm |
Tension |
Classifiers |
$$\sigma _{U}$$, $$MPa$$ |
$$\sigma_{P}$$, $$MPa$$ |
$$\epsilon_L$$, % |
$$\psi$$, % |
$$KCU\cdot 10^{3}$$, $$\frac{J}{m^2}$$ |
Treatment |
| Trumpet |
|
|
|
|
550 |
380 |
18 |
50 |
600 |
|
| Trumpet |
|
|
|
|
550 |
380 |
16 |
45 |
500 |
|
| Forgings |
|
|
|
|
640 |
450 |
17 |
50 |
500 |
|
Brinell hardness number
| Rolling |
Standard |
Classifiers |
Value, HBW |
| Alloy |
|
|
180–197 |
Critical point temperatures
| Ac1, K |
Ac3(Acm), K |
Ar3(Arcm), K |
| 780–830 |
1020–1040 |
830 |
Analogues
| Germany |
USA |
| GS-18 CrMo 9 10 |
A 757 Grade D1N1 |
Description of chemical elements
| Element |
Units of measurement |
Description |
| Fe |
% |
Iron |
| Si |
% |
Silicon |
| Mn |
% |
Manganese |
| Cr |
% |
Chrome |
| Cu |
% |
Copper |
| Ni |
% |
Nickel |
| V |
% |
Vanadium |
| P |
% |
Phosphorus |
| C |
% |
Carbon |
| S |
% |
Sulfur |
| Nb |
% |
Niobium |
| Mo |
% |
Molybdenum |
Description of physical characteristics
| Parameter |
Units of measurement |
Description |
| $$E\cdot 10^{9}$$ |
$$MPa$$ |
Elastic modulus |
| $$\alpha\cdot 10^{6}$$ |
$$K^{-1}$$ |
Coefficient of thermal (linear) expansion (range 20°C–T) |
| $$\varkappa$$ |
$$\frac{W}{m\cdot K}$$ |
Coefficient of thermal conductivity (the heat capacity of the material) |
| $$\rho$$ |
$$\frac{kg}{m^3}$$ |
The density of the material |
| $$R\cdot 10^{-6}$$ |
$$\Omega\cdot m$$ |
Electrical resistivity |
Description of mechanical properties
| Parameter |
Units of measurement |
Description |
| $$\sigma _{U}$$ |
$$MPa$$ |
Ultimate tensile strength |
| $$\sigma_{P}$$ |
$$MPa$$ |
Proportionality limit |
| $$\epsilon_L$$ |
% |
Elongation at break (longitudinal) |
| $$\psi$$ |
% |
Reduction in cross section on fracture |
| $$KCU\cdot 10^{3}$$ |
$$\frac{J}{m^2}$$ |
Impact toughness |
Description of temperatures of critical points
| Parameter |
Units of measurement |
Description |
| Ac1 |
K |
|
| Ac3(Acm) |
K |
|
| Ar3(Arcm) |
K |
|