Standard Fe, % Si, % Mn, % Ni, % Al, % P, % C, % S, % Mo, %
GOST 977-88 96.8–98.09 0.2–0.5 1.1–1.6 0.3–0.5 0.01 < 0.035 0.16–0.23 < 0.035 0.15–0.3

Information on suppliers

Mechanical properties at 20 °C

Rolling Standard Size, mm Tension Classifiers $$\sigma _{U}$$, $$MPa$$ $$\sigma_{Y}$$, $$MPa$$ $$\psi$$, % $$KCU\cdot 10^{3}$$, $$\frac{J}{m^2}$$ d5, % Treatment
Castings GOST 977-88 500 343 30 491 18 Normalization 880 - 920 ° C, Release 600 - 700 ° C

Режимы термической обработки

Обработка
Нормализация 880 - 920 ° C, Отпуск 600 - 700 ° C

Standards

Standard Description
GOST 977-88

Description of chemical elements

Element Units of measurement Description
Fe % Iron
Si % Silicon
Mn % Manganese
Ni % Nickel
Al % Aluminium
P % Phosphorus
C % Carbon
S % Sulfur
Mo % Molybdenum

Description of mechanical properties

Parameter Units of measurement Description
d5 % Elongation at break
$$\sigma_{Y}$$ $$MPa$$ Yield strength
$$\sigma _{U}$$ $$MPa$$ Ultimate tensile strength
$$\psi$$ % Reduction in cross section on fracture