EP61 (33CNMS)
Classification
| Country | Section | Category |
|---|---|---|
| CIS, Russia, Ukraine | Precision alloys | Soft Magnetic Precision Alloys |
Chemical composition
| Standard | Fe, % | Si, % | Mn, % | Co, % | Cr, % | Ni, % | P, % | C, % | S, % | Mo, % |
|---|---|---|---|---|---|---|---|---|---|---|
| 29.94–34.6 | 1.8–2.2 | 0.3–0.5 | 28–30 | < 0.1 | 32.5–34 | < 0.015 | < 0.03 | < 0.015 | 2.8–3.2 |
Information on suppliers
Physical characteristics
| Temperature, °C | $$E\cdot 10^{9}$$, $$MPa$$ | $$\rho$$, $$\frac{kg}{m^3}$$ | $$R\cdot 10^{-6}$$, $$\Omega\cdot m$$ |
|---|---|---|---|
| 20 | 185 | 8300–8320 | 0.7 |
Mechanical properties at 20 °C
| Rolling | Standard | Size, mm | Tension | Classifiers | $$\sigma _{U}$$, $$MPa$$ | $$\sigma_{Y}$$, $$MPa$$ | d5, % | Treatment |
|---|---|---|---|---|---|---|---|---|
| Tape | GOST 15515-16 | 100 | Transverse | 500–550 | 300–360 | 20–25 |
Magnetic properties
| Rolling | $$H_c$$, $$A/m$$ | $$\mu_{max}$$, $$MH/m$$ | $$B_{2500}$$, $$T$$ |
|---|---|---|---|
| Tape | < 13000 | < 5000 | > 32 |
Brinell hardness number
| Rolling | Standard | Classifiers | Value, HBW |
|---|---|---|---|
| Tape | GOST 15515-16 | 200–260 |
Свойства
| Свойство |
|---|
| В состоянии поставки обладает гарантируемым уровнем магнитных свойств в переменных полях |
Description of chemical elements
| Element | Units of measurement | Description |
|---|---|---|
| Fe | % | Iron |
| Si | % | Silicon |
| Mn | % | Manganese |
| Co | % | Cobalt |
| Cr | % | Chrome |
| Ni | % | Nickel |
| P | % | Phosphorus |
| C | % | Carbon |
| S | % | Sulfur |
| Mo | % | Molybdenum |
Description of physical characteristics
| Parameter | Units of measurement | Description |
|---|---|---|
| $$E\cdot 10^{9}$$ | $$MPa$$ | Elastic modulus |
| $$\rho$$ | $$\frac{kg}{m^3}$$ | The density of the material |
| $$R\cdot 10^{-6}$$ | $$\Omega\cdot m$$ | Electrical resistivity |
Description of mechanical properties
| Parameter | Units of measurement | Description |
|---|---|---|
| d5 | % | Elongation at break |
| $$\sigma_{Y}$$ | $$MPa$$ | Yield strength |
| $$\sigma _{U}$$ | $$MPa$$ | Ultimate tensile strength |
Description of magnetic properties
| Parameter | Units of measurement | Description |
|---|---|---|
| $$H_c$$ | $$A/m$$ | Magnetic coercivity (not more) |
| $$\mu_{max}$$ | $$MH/m$$ | Magnetic permeability (not more) |
| $$B_{2500}$$ | $$T$$ | Magnetic induction (not less) in a magnetic field while magnetic field strength is 2500 A/m |