15H18SYU (EI484, H18SYU)
tube pyrolysis plants, equipment, heat-resistant steel
Classification
| Country | Section | Category |
|---|---|---|
| CIS, Russia, Ukraine | Heat resistant steels and alloys | Heat resistant high alloy steel |
Chemical composition
| Standard | Fe, % | Si, % | Mn, % | Cr, % | Al, % | P, % | C, % | S, % |
|---|---|---|---|---|---|---|---|---|
| GOST 5632-72 | 76.29–81.3 | 1–1.5 | < 0.8 | 17–20 | 0.7–1.2 | < 0.035 | < 0.15 | < 0.025 |
Information on suppliers
Mechanical properties at 20 °C
| Rolling | Standard | Size, mm | Tension | Classifiers | $$\sigma _{U}$$, $$MPa$$ | $$\sigma_{P}$$, $$MPa$$ | $$\epsilon_L$$, % | $$\psi$$, % | Treatment |
|---|---|---|---|---|---|---|---|---|---|
| Rod | GOST 5949-75 | 490 | 295 | 20 | 50 | Annealing |
Analogues
| Germany | USA |
|---|---|
| 1.4742 | 430 |
Standards
| Standard | Description |
|---|---|
| GOST 5632-72 |
Description of chemical elements
| Element | Units of measurement | Description |
|---|---|---|
| Fe | % | Iron |
| Si | % | Silicon |
| Mn | % | Manganese |
| Cr | % | Chrome |
| Al | % | Aluminium |
| P | % | Phosphorus |
| C | % | Carbon |
| S | % | Sulfur |
Description of mechanical properties
| Parameter | Units of measurement | Description |
|---|---|---|
| $$\sigma _{U}$$ | $$MPa$$ | Ultimate tensile strength |
| $$\sigma_{P}$$ | $$MPa$$ | Proportionality limit |
| $$\epsilon_L$$ | % | Elongation at break (longitudinal) |
| $$\psi$$ | % | Reduction in cross section on fracture |