Alloy aluminum AK9ch (AL4)
Chemical composition
| Al | Aluminum | Rest |
| Fe | Iron | 0.3 — 1.0 |
| Si | Silicon | 8.0 — 10.0 |
| Mg | Magnesium | 0.35 — 0.55 |
| Mn | Manganese | 0.1 — 0.6 |
| Cu | Copper | 0.3 — 1.5 |
| Ni | Nickel | <0.3 |
| Zn | Zinc | 5.0 — 7.0 |
| Ot | Total impurities | <0.6 |
Pb + Sn <0.3
Analogs in Russia
AK9TS6 GOST 1583−93
AK9TS6r GOST 1583−93
AL12 GOST 2171−90
AK9TS6 GOST R 55375−12
for the manufacture of parts of medium and high load; the alloy is highly tight. Due to the increased propensity for gas saturation and the formation of porosity, crystallization under pressure is recommended for castings. Alloy based on the aluminum — silicon — magnesium system (silumin)
Classification
| Country | Section | Category |
|---|---|---|
| CIS, Russia, Ukraine | Aluminum, aluminum alloys | Foundry aluminum alloys |
Chemical composition
| Standard | Fe, % | Si, % | Be, % | Sn, % | Mg, % | Mn, % | Cu, % | Zn, % | Ni, % | Al, % | Pb, % |
|---|---|---|---|---|---|---|---|---|---|---|---|
| GOST 1583-93 | < 1 | 8–10.5 | < 0.1 | < 0.01 | 0.17–0.3 | 0.2–0.5 | < 0.3 | < 0.3 | < 0.1 | 86.84–91.63 | < 0.05 |
Information on suppliers
Physical characteristics
| Temperature, °C | $$E\cdot 10^{9}$$, $$MPa$$ | $$\alpha\cdot 10^{6}$$, $$K^{-1}$$ | $$\varkappa$$, $$\frac{W}{m\cdot K}$$ | $$\rho$$, $$\frac{kg}{m^3}$$ | $$c\cdot 10^{-3}$$, $$\frac{J}{kg\cdot K}$$ | $$R\cdot 10^{-6}$$, $$\Omega\cdot m$$ |
|---|---|---|---|---|---|---|
| 20 | 0.7 | 2650 | 46.8 | |||
| 100 | 21.7 | 155 | 755 |
Mechanical properties at 20 °C
| Rolling | Standard | Size, mm | Tension | Classifiers | $$\sigma _{U}$$, $$MPa$$ | d5, % | Treatment |
|---|---|---|---|---|---|---|---|
| Chill casting | GOST 1583-93 | 235 | 3 | Hardening and artificial aging | |||
| Chill casting | GOST 1583-93 | 147 | 2 |
Brinell hardness number
| Rolling | Standard | Classifiers | Value, HBW |
|---|---|---|---|
| Heat-treated steel. | GOST 1583-93 | 50–70 |
Analogues
| USA | Germany |
|---|---|
| 360 | G-AlSi10Mg |
Description of chemical elements
| Element | Units of measurement | Description |
|---|---|---|
| Fe | % | Iron |
| Si | % | Silicon |
| Be | % | Beryllium |
| Sn | % | Tin |
| Mg | % | Magnesium |
| Mn | % | Manganese |
| Cu | % | Copper |
| Zn | % | Zinc |
| Ni | % | Nickel |
| Al | % | Aluminium |
| Pb | % | Lead |
Description of physical characteristics
| Parameter | Units of measurement | Description |
|---|---|---|
| $$E\cdot 10^{9}$$ | $$MPa$$ | Elastic modulus |
| $$\alpha\cdot 10^{6}$$ | $$K^{-1}$$ | Coefficient of thermal (linear) expansion (range 20°C–T) |
| $$\varkappa$$ | $$\frac{W}{m\cdot K}$$ | Coefficient of thermal conductivity (the heat capacity of the material) |
| $$\rho$$ | $$\frac{kg}{m^3}$$ | The density of the material |
| $$c\cdot 10^{-3}$$ | $$\frac{J}{kg\cdot K}$$ | The specific heat of the material (range 20°C–T) |
| $$R\cdot 10^{-6}$$ | $$\Omega\cdot m$$ | Electrical resistivity |
Description of mechanical properties
| Parameter | Units of measurement | Description |
|---|---|---|
| d5 | % | Elongation at break |
| $$\sigma _{U}$$ | $$MPa$$ | Ultimate tensile strength |