Chemical composition
| Standard | Fe, % | Si, % | Be, % | Mg, % | Mn, % | Ti, % | Cu, % | Zn, % | Zr, % | Al, % |
|---|---|---|---|---|---|---|---|---|---|---|
| GOST 1583-93 | < 0.05 | < 0.05 | 0.02–0.1 | 6–7 | < 0.1 | 0.05–0.15 | < 0.05 | < 0.05 | 0.05–0.2 | 92.25–93.88 |
Information on suppliers
Mechanical properties at 20 °C
| Rolling | Standard | Size, mm | Tension | Classifiers | $$\sigma _{U}$$, $$MPa$$ | d5, % | Treatment |
|---|---|---|---|---|---|---|---|
| Castings | GOST 1583-93 | 196–245 | 5–10 |
Brinell hardness number
| Rolling | Standard | Classifiers | Value, HBW |
|---|---|---|---|
| Alloy | GOST 1583-93 | 60 |
Analogues
| USA |
|---|
| 535 |
Standards
| Standard | Description |
|---|---|
| GOST 1583-93 | |
| GOST Р 55375-2012 | |
| DSTU 2839-94 |
Description of chemical elements
| Element | Units of measurement | Description |
|---|---|---|
| Fe | % | Iron |
| Si | % | Silicon |
| Be | % | Beryllium |
| Mg | % | Magnesium |
| Mn | % | Manganese |
| Ti | % | Titan |
| Cu | % | Copper |
| Zn | % | Zinc |
| Zr | % | Zirconium |
| Al | % | Aluminium |
Description of mechanical properties
| Parameter | Units of measurement | Description |
|---|---|---|
| d5 | % | Elongation at break |
| $$\sigma _{U}$$ | $$MPa$$ | Ultimate tensile strength |